All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Lithium Carbonate 1.00
Nepheline Syenite 60.00
Strontium Carbonate 20.00
OM 4 Ball Clay 10.00
Silica 9.00
Add Amount
Titanium Dioxide 5.00
Silicon Carbide 2.50

Instructions


I use this as a base glaze and have added a variety of stains. Different stains cause the craters to expand more, particularly red and yellow. I also get larger craters with faster firing. I apply it thickly with a brush.

This recipe was shared by Jill Birschbach in the September 2020 issue of Ceramics Monthly.