All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Gerstley Borate 13.40
Dolomite 5.90
Whiting 8.30
Zinc Oxide 4.00
F-4 Feldspar 46.20
EPK Kaolin 2.40
Silica 19.80
Add Amount
Black Copper Oxide 4.00

Instructions