All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Gerstley Borate 26.00
Lithium Carbonate 4.00
Ferro Frit 3124 30.00
Nepheline Syenite 20.00
EPK Kaolin 10.00
Silica 10.00
Add Amount
Vee Gum 2.00
CMC Gum 1.00

Instructions

Published in the March 2018 issue of Ceramics Monthly.
Note: Vee gum (for brushability) and CMC gum (to harden the glaze surface before firing) need to be blunged in hot water before being added to the glaze. To keep measurements accurate, use a ratio of 1g CMC or Vee gum to 19g water. For every gram needed in the glaze, measure out 20g of the mixed solution. The commercial stains listed are Mason stains (MS) from Mason Color Works (www.masoncolor.com).

The following color variations can be made with this base:

For A-23 Iron Yellow, Add: 4% Red Iron Oxide, 2% MS 6450 Praseodymium Yellow Stain.

For A-22 Water Blue, Add: 2% Copper Carbonate, 2% MS 6450 Praseodymium Yellow Stain.

For PG E, Add: 4% MS 6263 Victoria Green.

For PG 1 Lavender, Add: 6% MS 6319 Lavender.

For PG B Light Blue, Add: 4% Turquoise Stain.

For PG F Dark Cobalt Blue, Add 2% Cobalt Carbonate.

For PG G Cobalt Blue, Add: 0.5% Cobalt Carbonate.