All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Lithium Carbonate 3.00
Strontium Carbonate 9.00
Ferro Frit 3110 59.00
EPK Kaolin 12.00
Silica 17.00
Add Amount
Red Iron Oxide 6.00

Instructions

This recipe was originally published in the January/February 2018 issue of Pottery Making Illustrated.
This glaze isn’t stable (it’s very fluid), but when used in accent areas it forms nice pools and drips. Crackle glaze isn’t suitable for food surfaces.