All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Lithium Carbonate 3.00
Strontium Carbonate 9.00
Ferro Frit 3110 59.00
EPK Kaolin 12.00
Silica 17.00
Add Amount
Red Iron Oxide 6.00

Instructions

Published in "Emerging Glazes," in the May 2016 issue of Ceramics Monthly, page 86.

I use this glaze in accent areas as it forms nice pools and drips. This is a runny reactive glaze so when I am making a piece, I always have this in mind and make little catchment areas for it to pool and drip. This glaze is not food safe.
I apply this glaze with a brush and more often than not, layer and blend it with other glazes. This glaze is not food safe.