All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Dolomite 3.01
Whiting 10.23
Borax Frit 16.55
Potash Feldspar 44.38
Kaolin 1.25
Silica 24.58
Add Amount
Tin Oxide 0.80
Copper Carbonate 1.00

Instructions

Published in "Vincent Beague" by Nesrin During, in the Oct 2001 issue of Ceramics Monthly.
This image shows a Temmoku glaze, fired to 2336 degrees Fahrenheit (1280 degrees Celsius), then warmed and glazed with the Oxblood Glaze fired in reduction to 2336 degrees Fahrenheit (1280 degrees Celsius).