All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Ferro Frit 3124 5.00
Nepheline Syenite 15.00
Talc 30.00
Calcined EPK Kaolin 10.00
OM4 Ball Clay 30.00
EPK Kaolin 10.00
Add Amount
Superpax 5.00

Instructions

Published in "Throw, Cut and Paste" by Joan Bruneau, in the Nov/Dec 2010 issue of Pottery Making Illustrated.
For use with wet to leather-hard clay.