All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Bone Ash 11.00
Talc 10.00
Soda Feldspar 52.00
Kaolin 5.00
Silica 22.00
Add Amount
Red Iron Oxide 5.00

Instructions


This recipe was sourced from The Ceramic Spectrum: A Simplified Approach to Glaze and Color Development by Robin Hopper.