All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Bone Ash 1.10
Talc 7.80
Whiting 22.40
Custer Feldspar 30.90
EPK Kaolin 12.50
Silica 25.30
Add Amount
Copper Carbonate 5.50
Bentonite 1.00

Instructions


I fire this glaze up to cone 11–12 on heavy reduction in a wood kiln, but it also works fine fired in a gas kiln to cone 10 in normal reduction.

This recipe was shared by Monte Young in the March 2020 issue of Ceramics Monthly.