All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Bone Ash 1.05
Talc 7.81
Whiting 22.36
Custer Feldspar 30.91
EPK Kaolin 12.55
Silica 25.32
Add Amount
Bentonite 2.50
Copper Carbonate 5.50

Instructions

Image shown is porcelain, Bauer Orange Flashing Slip, commercial underglaze, Oribe Green, soda fired to cone 10-11.

Published in "Soda Surfaces" by Nolan Baumgartner, in the Dec 2014 issue of Ceramics Monthly.