All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Dolomite 21.41
Lithium Carbonate 1.02
Ferro Frit 3124 10.19
Nepheline Syenite 62.18
OM4 Ball Clay 5.20
Add Amount
Tin 8.15
Rutile 7.14
Spanish Iron Oxide 6.12
Bentonite 2.04

Instructions

This recipe was shared by Ernest Miller is the January/February 2019 issue of Pottery Making Illustrated.
This glaze fires bright orange on white clay while firing dark orange-brown on an iron-bearing clay.