All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Whiting 19.00
Zinc Oxide 9.00
G200 Feldspar 52.00
EPK Kaolin 15.00
Silica 5.00
Add Amount
Zircopax Plus 10.00
Mason Stain 10.00
Bentonite 1.00

Instructions


I program a 15-minute hold and slow cool at the end of the firing in an electric kiln. This gives a very soft matte finish with little sheen. Otherwise it is a bit waxy with a low sheen. I used Mason stain #6315 Zirconium Vanadium Blue as the colorant in the process images.

This recipe was shared by Alan Johnson in the January/February 2021 issue of Pottery Making Illustrated.