All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Dolomite 21.50
Gerstley Borate 11.00
Nepheline Syenite 64.90
OM 4 Ball Clay 2.60
Add Amount
Zircopax 16.20
Red Iron Oxide 1.00
Bentonite 2.20

Instructions

Published in "Working Potter Glazes" in the June 2015 issue of Ceramics Monthly.

Old White is a matte off-white surface when applied in a single coat and is a glossy warm white in a double coat. It's a finicky glaze to apply, it will crawl if it is applied too thick or if multiple layers are applied too quickly. The glaze flashes any clay left raw next to a glazed surface area.
Mix all ingredients together prior to adding the water.