All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Custer Feldspar 15.00
Tile 6 Kaolin 40.00
OM 4 Ball Clay 30.00
Silica 15.00

Instructions

White to toasty brown/orange in a cone 6 soda firing. Works well in a wide temperature range in oxidation and reduction.

Published in "Low-Fire Surfaces" by Ronan Kyle Peterson, in the September 2017 issue of Ceramics Monthly.
I apply one coat of Oestreich White Slip using dipping or pouring methods.