All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Soda Ash 4.00
Spodumene 15.00
Kona F-4 Feldspar 11.00
Nepheline Syenite 45.00
EPK 10.00
OM-4 Ball Clay 15.00

Instructions

Burnt orange shino when single dipped, greyish-white when applied thicker. (fired at cone 9-11)  Some crazing occurs when thickly applied.

Source: American Shino (Book) - Jeff Oestreich
Test batch was mixed by hand.  Test tile dipped fully once and half-dipped a second time.