All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Gerstley Borate 20.00
Wollastonite 10.00
Nepheline Syenite 30.00
EPK Kaolin 10.00
Silica 30.00

Instructions


A clear glaze designed to fire at cone 5 or 6. I fire it to cone 4 on Highwater Clay’s Earthen Red clay body and it works wonderfully. The fired results are best when the specific gravity is 1.4. If applied too thick, it can result in crawling or create a foggy look on top of underglaze.

This recipe was shared by Sara Ballek in the November/December 2020 issue of Pottery Making Illustrated.