All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Barium Carbonate 13.55
Whiting 15.81
Custer Feldspar 54.19
EPK Kaolin 12.26
Silica 4.19
Add Amount
Red Iron Oxide 2.00
Rutile 7.97

Instructions


This breaking glaze is beautiful for sculptural works, but isn't advised for contact with food.