All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Oak Ash 52.00
Cornwall Stone 16.00
Custer Feldspar 16.00
Grolleg Kaolin 6.00
XX Saggar 3.00
Silica 7.00
Add Amount
Red Iron Oxide 5.00
Veegum T 1.00

Instructions


I fire this glaze in reduction to cone 9 in the wood kiln. The oak ash is unwashed before use.

This recipe was shared by Jeff Diehl in the May 2020 issue of Ceramics Monthly.