All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Dolomite 23.00
Spodumene 23.00
Ferro Frit 3134 7.70
Redart 13.30
EPK Kaolin 9.70
Silica 23.30
Add Amount
Red Iron Oxide 0.50
Yellow Ochre 3.20
Tin Oxide 4.90
Bentonite 2.00

Instructions

Published in "Nutmeg Remix" by Deklan Ranlett, in the Jul/Aug 2012 issue of Pottery Making Illustrated.
This Nutmeg glaze version has a nice break of cream coming from the tin and the color was very rich using both iron and Redart.