All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Gerstley Borate 14.20
Whiting 11.70
Nepheline Syenite 50.60
Grolleg Kaolin 5.00
Silica 18.50
Add Amount
Praseodymium Oxide 7.50

Instructions

Originally published in the November 2017 issue of Ceramics Monthly.
0.05% CMC gum can be added to this glaze to help prevent it from settling. This glaze has some opacity/ satin character.