All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
#6 Tile Kaolin 20.00
EPK Kaolin 16.00
Grolleg Kaolin 9.00
OM 4 Ball Clay 4.00
Minspar 200 Feldspar 21.50
Pyrophyllite 1.50
Silica 28.00
Add Amount
Vee Gum T 1.15

Instructions

This porcelain clay body is suitable for both wheel throwing and hand building.

Originally published in the December 2017 issue of Ceramics Monthly.