All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Dolomite 7.46
Whiting 4.38
Ferro Frit 3134 24.54
Nepheline Syenite 25.50
EPK Kaolin 17.31
Silica 20.81
Add Amount
Mason Stain 6129 Golden Ambrosia 3.00
Mason Stain 6318 Amethyst 2.00
Mason Stain 6373 Turquoise 2.00
Mason Stain 6242 Bermuda Green 3.00

Instructions


This is my base glaze, a clear that I add Mason stains to as needed. It's made to fit well on Standard 365 porcelain, and runs a little bit to make underglazes bleed. All the bold color work on my pots is done with Speedball underglazes.

This recipe was shared by Neil Estrick in the February 2020 issue of Ceramics Monthly.