All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Gillespie Borate 30.00
Ferro Frit 3195 30.00
Nepheline Syenite 20.00
EPK Kaolin 10.00
Silica (325 mesh) 10.00
Add Amount
Copper Carbonate 5.00

Instructions


Test with 5–8% copper carbonate.

This recipe was shared by Nathan Bray in Low-Fire Soda by Justin Rothshank, available through the Ceramic Arts Network shop: https://mycan.ceramicartsnetwork.org/s/product-details?id=a1B3u000009udqwEAA.