All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Custer Feldspar 5.00
Cedar Heights Redart 19.00
Newman Red Clay 14.00
Stancills Red Clay 38.00
Tennessee #10 Ball Clay 24.00
Add Amount
Bentonite 1.00
Medium Grog 10.00

Instructions


Stancills Red Clay is a clay I source from a local mine. This is a great throwing body that fires dark brown in reduction.