All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Gerstley Borate 14.05
Strontium Carbonate 1.11
Whiting 16.88
Ferro Frit 3195 7.63
Custer Feldspar 15.31
EPK Kaolin 16.51
Silica 28.51
Add Amount
Bentonite 2.00

Instructions


This base takes stains really well. I use up to 9% stain for fully saturated color swatches and smaller sections of glaze that I paint on, and 1–3% stain in my liner glaze palette choices. This recipe was shared by Richard Burkett in San Diego, California.

This recipe was shared by Deb Schwartzkopf in the March 2019 issue of Ceramics Monthly.