All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Barium Carbonate 1.98
Gerstley Borate 6.46
Lithium Carbonate 11.26
Magnesium Carbonate 2.82
Whiting 12.39
Nepheline Syenite 23.61
Silica 41.48
Add Amount
Tin Oxide 3.05
Dark Rutile 3.55

Instructions


Specific gravity: 1.40. Of these recipes, Nancy’s Pink Icing was the most difficult to get a good test. I tested it on white and brown stoneware with noticeable color response differences. The surface is a pleasing silk matte and is completely opaque. Extreme accuracy is required when mixing to result in a strong pink.

Original recipe shared by Harold McWhinnie in the January 1982 issue of Ceramics Monthly.