All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Gillespie Borate 30.00
F-4 Feldspar (sub G200 Feldspar) 46.00
EPK Kaolin 13.00
Silica 11.00
Add Amount
Copper Carbonate 1.00
Titanium Dioxide 1.00

Instructions


The addition of titanium dioxide makes this glossy slightly opaque.

This recipe was shared by Yoko Sekino-Bové in the April 2021 issue of Ceramics Monthly.