All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
F-4 Feldspar 3.80
Nepheline Syenite 2.00
Cornwall Stone 40.30
Whiting 6.50
Silica 17.80
Gerstley Borate 2.60
Magnesium Carbonate 3.20
Barium Carbonate 1.30
Wood Ash 18.90
Zinc Oxide 3.70
Add Amount
Tin Oxide 3.20
Black Copper Oxide 1.90

Instructions


Nice purple color