All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
G200-EU Potash Feldspar 17.50
C&C Ball Clay 60.00
Grolleg Kaolin 5.00
Silica (400 Mesh) (Supersil) 17.50

Instructions


Allow slip to soak in water overnight before sieving to avoid lumps. Sieve through 80-mesh screen, then through a 100-mesh screen (do not screen through a 120-mesh screen). If too fine, it won’t adhere to the clay or glaze as well.

This recipe was shared by Miranda Thomas in the October 2020 issue of Ceramics Monthly.