All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Bone Ash 2.30
Dolomite 6.90
Whiting 11.49
G200-EU Potash Feldspar 45.98
Grolleg Kaolin 5.74
Silica (400 Mesh) (Supersil) 27.59
Add Amount
Red Iron Oxide 1.72
Bentonite 1.72

Instructions


Mix to a single cream consistency. This glaze works well over Miranda Thomas Black Slip. Note: G200-EU Potash Feldspar is manufactured in Spain.

This recipe was shared by Miranda Thomas in the October 2020 issue of Ceramics Monthly.