All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Gerstley Borate 77.80
Lithium Carbonate 22.20
Add Amount
Chrome Oxide 0.30
Manganese Dioxide 44.40
Copper Carbonate 6.70

Instructions

Metallic Platinum can been seen on the raised bumps in the image shown on this page.

Published in "Studio Takada" by Kaname and Sumiko Takada, in the March 2017 issue of Ceramics Monthly.
This glaze shifts slightly at cone 05.