All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Nepheline Syenite 45.00
Strontium Carbonate 26.00
Kentucky Ball Clay (OM 4) 13.00
Silica 8.00
Copper Carbonate 2.00
Rutile 3.00
Bentonite 3.00
Add Amount
Epsom Salt 0.25

Instructions


Nice even matte