All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Gerstley Borate 10.20
Strontium Carbonate 15.20
Wollastonite 15.20
Nepheline Syenite 38.70
EPK Kaolin 10.20
Silica 10.50

Instructions

Good satin-matte clear/base that holds colorants exceptionally well. Try testing this base with the addition of other oxides, carbonates, and commercial stains to achieve different colors.

Published in "Mid-Range Glazes" by Forrest Sincoff Gard, in the April 2017 issue of Ceramics Monthly.