All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Gerstley Borate 42.31
Whiting 23.08
EPK Kaolin 23.07
Silica 11.54
Add Amount
Mason stain #6600 10.00
Zircopax 3.85

Instructions

A liner glaze that doesn't shift or move at cone 05. It works well for dipping, pouring, and brushing.

Published in "Studio Takada" by Kaname and Sumiko Takada, in the March 2017 issue of Ceramics Monthly.