All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Strontium Carbonate 10.00
Talc 2.00
Ferro Frit 3134 27.00
Nepheline Syenite 30.00
EPK Kaolin 13.00
Silica 18.00
Add Amount
Bentonite 2.00
Zircopax 6.00
Bermuda Green Mason Stain 4.00

Instructions

Published in "Low-fire to cone 3 Recipes," in the September 2018 issue of Ceramics Monthly.

The image shown here has multiple glazes on it. This is the second color addition.

I use this as a liner glaze. Apply thinly for clear. For opaque colors, mix to a heavy-cream consistency for a thicker application.