All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Strontium Carbonate 10.00
Talc 2.00
Ferro Frit 3134 27.00
Nepheline Syenite 30.00
EPK Kaolin 13.00
Silica 18.00
Add Amount
Bentonite 2.00

Instructions


Mix the glaze to a whole-milk consistency. The thinnest possible layer is recommended for most low-fire clear glazes; however, a standard 3-second count application of this glaze works best. It takes colorants well and works over underglazes and terra sigillatas.

This recipe was shared by Marty Fielding in the in the December 2020 issue of Ceramics Monthly.