All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Lithium Carbonate 7.10
Whiting 12.90
Ferro Frit 3134 40.50
EPK Kaolin 21.70
Silica (325 mesh) 17.80
Add Amount
Copper Carbonate 3.00

Instructions

Published in "Low-Fire Alkaline Glazes" by Cheryl Pannabecker, in the May/Jun 2011 issue of Pottery Making Illustrated.