All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Barium Carbonate 9.00
Gerstley Borate 2.50
Lithium Carbonate 2.50
Strontium Carbonate 9.50
Wollastonite (Calcium Silicate) 1.00
Ferro Frit 3110 13.00
Nepheline Syenite 14.00
Grolleg 11.50
Silica 37.00
Add Amount
Bentonite 2.00
Black Nickel Oxide 1.00
Cobalt Carbonate 0.25

Instructions

Published in "Andrew Martin's Aquatic Aesthetic" by Glen R. Brown, in the Jan 2011 issue of Ceramics Monthly.


The variety of fluxes in this glaze help to promote a wide range of colors. In order to get French Chartreuse, Maroon, Orchard Purple, and Aegean Blue, this exact recipe should be followed. Some of the other colors can be made by substituting strontium carbonate for the barium (removing barium and using 18.5% strontium carbonate total). Do small tests to see if the colorant combination you want to use responds well to this change.

Originally, this was a cone 10 glaze, but it can be fired to cone 6 with a 30 minute soak (effectively a cone 7 1/2 firing), and still achieve glossy results.

Dripping is the best method for applying this glaze, as pouring and spraying can lead to uneven coatings, resulting in prominent lines on the finished work.

At cone 10, the glaze is more fluid, so be sure not to apply it too thickly (not more than the thickness of a dime), and wax 1/8 to 1/4 inch up from the foot or base of your piece.

Bright colors can be achieved over a white surface. The color of your clay will dramatically affect the color of the finished, fired glaze.

The glaze has a tendency to crackle or craze over many clay bodies.