All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Custer Feldspar 45.00
Zinc Oxide 2.25
Dolomite 2.00
Colemanite 10.00
Whiting 9.00
Flint 25.00
Add Amount
Copper Carbonate 1.00
Tin Oxide 1.00
Red Iron Oxide 0.50
Barium Carbonate 0.50

Instructions

This is a glaze from Mark Talbert (Utah Valley University).

The test tile is Coleman Porcelain fired in reduction.
It will run if applied thickly.  For good color, reduce early.