All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Borax 3.88
Gerstley Borate 46.51
Magnesium Carbonate 31.01
EPK Kaolin 18.60

Instructions

When fired to cone 04, it has a glassy bead-like effect. When applied thinly and fired to cone 06, the glaze crawls into small, dry platelets, creating a lichen look. If thickly applied, the platelets are larger and the distance between greater, similar to a dry river bottom.

Published in "Accentuating Form with Glaze" by Mary Fox, in the January/February 2017 issue of Pottery Making Illustrated. Originally from Mark Messenger's notes, Ceramics Monthly May 1996.

 
For White: add 5.43% Zircopax.

For Green: add 1–5% Copper Carbonate

For Blue/Purple: add 1–5% Cobalt Carbonate