All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Dolomite 4.70
Lithium Carbonate 2.00
Talc 8.00
Whiting 15.90
Custer Feldspar 20.20
Grolleg Kaolin 18.90
Silica 30.30
Add Amount
Tin Oxide 3.50

Instructions


Mix to a cream-like consistency and apply thickly by pouring or dipping. This glaze breaks on edges and throwing lines.

This recipe was shared by Patrick Yeung in the December 2019 issue of Ceramics Monthly.