All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Dolomite 23.40
Whiting 2.13
G-200 Feldspar 31.91
Spodumene 21.28
EPK Kaolin 21.28
Add Amount
Tin Oxide 6.38

Instructions


Apply thick by dipping or pouring in and out if just used as liner. I fire this glaze to cone 11 in a wood kiln with heavy reduction. Fly ash in the firing can cause gray to pink speckling.

This recipe was shared by Scott McClellan in the October 2019 issue of Ceramics Monthly.