All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Whiting 19.00
Custer Feldspar 45.50
EPK Kaolin 10.00
Silica 25.50
Add Amount
Spanish Red Iron Oxide 1.00

Instructions


This is one of the only fool-proof glazes I have found that works in reduction cooling. A beautiful blue celadon that brightens up and becomes more translucent around cone 10, and takes on the characteristics of a traditional semi-opaque, or milky celadon at cone 9.

This recipe was shared by Forrest Lesch-Middelton in the October 2020 issue of Ceramics Monthly.