All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Lithium Carbonate 6.00
Ferro Frit 3110 80.00
EPK Kaolin 4.00
Silica 10.00
Add Amount
Bentonite 2.00
CMC Gum 0.60
Veegum T 1.80
Copper Carbonate 2.50

Instructions

Originally published in the May 2018 issue of Ceramics Monthly.
Brush 3–5 even coats onto work. The glaze can be very runny depending on thickness and hold time at top temperature. Mix in small batches as glaze can settle out and gel very quickly.