All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Lithium Carbonate 6.00
Ferro Frit 3110 80.00
EPK Kaolin 4.00
Silica 10.00
Add Amount
CMC Gum 0.60
Veegum T 1.80
Bentonite 2.00
Copper Carbonate 2.50
Iron Chromate 0.50

Instructions


Brush 3–5 even coats onto work. Fire to cone 04. Glaze can be very runny depending on thickness and hold at top temperature. Because this glaze can gel, I add a couple of drops of Darvan and only mix it in small batches.

This recipe was shared by Mike Gesiakowski in the July/August 2019 issue of Pottery Making Illustrated.