All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Dolomite 12.96
Lithium Carbonate 1.85
Whiting 14.81
Custer Feldspar 33.33
EPK Kaolin 5.57
Silica 31.48

Instructions

Published in "Cone 6-10 Glazes" in the Jan 2015 issue of Ceramics Monthly.

Great liner glaze when satin-coffee and tea will not stain it. In reduction, it is a bit blue.
Do not eliminate lithium or the glaze will settle. I use 1.85% lithium, but up to 3.7% will work. Fire to cone 9 to get a satin finish.