All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Talc 4.04
Wollastonite 7.07
Nepheline Syenite 3.03
Cedar Heights Goldart 10.10
Cedar Heights Redart 65.66
OM 4 Ball Clay 10.10
Add Amount
Barium Carbonate 0.51
Bentonite 1.01

Instructions


Add barium carbonate to prevent scumming.

This recipe was shared by Lisa Naples in the November 2020 issue of Ceramics Monthly.