All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Nepheline Syenite 32.00
OM 4 Ball CLay 63.00
Silica 5.00
Add Amount
Titanium Dioxide 5.00
Zircopax 6.00

Instructions


Mix this slip to skim milk consistency. Apply a very this coat to bisque-fired ware to prevent adhesion issues. The fired color range is bright yellow to orange brown. I use this slip on pieces placed throughout the wood kiln. I tend to put slipped pieces in areas where there will be more ash, and glazes pieces in cooler parts of the kiln with less ash exposure.

This recipe was share by Lisa York in the April 2020 issue of Ceramics Monthly.