All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Whiting 20.00
Custer Feldspar 40.00
EPK Kaolin 10.00
Silica 30.00
Add Amount
Superpax 5.00
Bentonite 2.00
CMC Gum 0.20

Instructions


This bluish-white glaze that is on the pot shown here is achievable only in cone-10 reduction soda firing. When used in other atmospheres, the fired result is a shiny white.