All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Water* (in pounds) 100.00
Clay (dry, in pounds) 50.00
Add Amount
Deflocculant** 0.25

Instructions


*100 pounds of water is 12 1/2 gallons.

**For this batch size, use 1/2 to 3/4 cup defloccuant.

This recipe yields about 7 gallons of terra sigillata.

This recipe was shared by Rhonda Willers in the February 2021 issue of Ceramics Monthly, sourced from Terra Sigillata: Contemporary Techniques by Rhonda Willers.